Chromium Trioxide in Metal Surface Treatment
Decorative versus hard chrome
Decorative chrome is a thin (0.1–1 μm) bright deposit over nickel; the bath is held around 250 g/L CrO₃ at 40–50 °C and the catalyst balance decides brightness and coverage. Hard chrome is 2–500 μm of functional coating valued for wear resistance and low friction; it runs at 50–60 °C and higher current density, and bath impurities show up as roughness and burning.
In both cases the impurity that accumulates fastest is sulfate from drag-in and from the chromic acid itself, which is why plating shops specify 0.03% or lower sulfate in the flake they buy.
Passivation and conversion coatings
Chromate conversion coatings use dilute chromic acid with activators to leave a thin Cr(III)/Cr(VI) film that passivates zinc, aluminium and cadmium surfaces. CrO₃ concentration and pH control film thickness and colour, from clear blue to yellow iridescent.
Grade recommendation
- Aerospace and precision hard chrome → electrolytic crystal (≥99.9%, sulfate ≤0.005%)
- Decorative plating with tight colour control → Superior flake (≥99.8%)
- High-throughput shops that top up continuously → First or Qualified flake
Frequently asked questions
Which CrO₃ grade is best for hard chrome plating?
Electrolytic crystal (CrO₃ ≥99.9%, sulfate ≤0.005%) or Superior sulfate flake (≥99.8%, sulfate ≤0.03%). Lower sulfate gives brighter, crack-free deposits and longer bath life.
What sulfate level should a plating bath hold?
The classic chromic-acid-to-sulfate ratio is about 100:1 by weight. Buying flake with ≤0.03% sulfate makes that ratio easier to hold as the bath is topped up.
Can chromium trioxide be used for trivalent chrome processes?
No — trivalent processes use chromium(III) salts. CrO₃ is a Cr(VI) product and belongs to hexavalent plating and chromate conversion chemistry.